I have experienced uneven etching using CuCl too. I etch my boards horizontally facing up, and the etching happens from the edge to the center of the board, and takes about 30minutes to have an 8x6" board done. The end result is perfect and the traces look fine, although I'm a bit concerned about the time too. I think my mix needs more oxigen too.

Fp
www.tonepad.com




  ----- Original Message ----- 
  From: grantfair2001 
  To: Homebrew_PCBs@yahoogroups.com 
  Sent: Sunday, May 04, 2003 9:59 PM
  Subject: [Homebrew_PCBs] First pcb etched with CuCl


  Even though my tank of etchant is far from the deep green color which
  shows it is at an optimum, I decided to etch a small board tonight. I
  hung it in the etchant above the aerator. (I drilled  a hole in one
  end and hung it from an insulated wire).

  In about 25 minutes one half (the part closest to the etchant surface)
  was etched clear. It took another 25 minutes to get the other half
  clear. I finally had to hang it upside down to get it cleared. A
  horizontal pcb holder is in the planning stages.

  In the first 20 minutes or so, I noticed part of the copper on the PCB
  was light grey in color. I suspect this was CuCl(I) because when I put
  a small amount of green etchant from the tank lid on this area, it
  disappeared. This also suggests that there is lots of CuCl(I) still in
  solution.

  I measured the pH again with indicator paper. The paper showed red (2)
  after I emptied the second 4 litre jug of HCl into it a few days ago.
  However, today it was 3 (or higher, if the the pH is higher yet and
  the etchant is discoloring the indicator paper).

  Although there is green etchant on the inner surface of the tank top,
  a drop of tank etchant dropped on the same lid is dark brown. So a lot
  of CuCl(I) needs to be converted. I am waiting for some fine bubble
  diffuser hose. Unfortunately most fish farming is done on the east and
  west coasts of Canada, and I am more or less in the middle between the
  two.

  So things are progressing, if slowly, I am learning about the CuCl
  approach, and I have etched my first board. In spite of the long dunk
  it looks just fine with all traces intact. Because I haven't had a
  totally clear recipe to operate from, things have gone slowly. But I
  hope my experience will make it easier for anyone who wants to use
  this appraoch in the future.

  Grant


        Yahoo! Groups Sponsor 

             
       
       

  Be sure to visit the group home and check for new Bookmarks and files:
  http://groups.yahoo.com/group/Homebrew_PCBs

  To unsubscribe from this group, send an email to:
  Homebrew_PCBs-unsubscribe@yahoogroups.com



  Your use of Yahoo! Groups is subject to the Yahoo! Terms of Service. 



[Non-text portions of this message have been removed]

Attachments

Move to quarantaine

This moves the raw source file on disk only. The archive index is not changed automatically, so you still need to run a manual refresh afterward.